Preparation of Novel Membrane Distillation Membranes with Facile and Cost-Effective Methods
Author:
Abstract:
To relieve the pressure related to water scarcity in the current generation, desalination is entrusted with an important mission. Compared to the traditional desalination technologies including thermal distillation and reverse osmosis, membrane distillation (MD) has its own advantages such as mild operation conditions, a high rejection of salts, less sensitive to the feed concentration, the feasibility of low-grade heat resources, and great potential application in small scale systems. As the physical barrier to separate the hot feed solution and cool permeate side and provide the space for vapor transport while rejecting nonvolatile matters in the feed, the membrane is essential to ensure a high MD performance in terms of flux, rejection, and anti-wetting properties. Plenty of efforts have been made to fabricate MD membranes including non-solvent induced phase separation, electrospinning, combined with post modifications such as blending, coating, grafting, plasma modification, nanoimprinting. However, the complicated processing procedure and the high cost of chemicals as well as possible toxicity are major obstacles to scale up the available membranes. Therefore, exploring simple, efficient, and cost-effective membrane preparation methods is extremely important. In this thesis, three methods are discussed. Firstly, the feasibility of using 3D printed (3DP) membranes in membrane distillation (MD) is explored for the first time in this work. Polyamide (PA) membranes were printed by a laser sintering (LS) technology, and further coated with thin poly(vinylidene fluoride) (PVDF) layers to reduce the pore size by dip-coating. The impact of PVDF concentration and immersion time on the membrane morphology, hydrophobicity, pore size, porosity, and DCMD performance were investigated. Results show that the additional PVDF layers could effectively reduce the membrane pore size from 15.9±5.3 μm to 1.0-2.5 μm. Additionally, due to the granular and rough surface of the 3DP substrates formed by the coalescence of PA powders, the hydrophobicity of the composite membranes (100°-130°) was greater than for the conventional PVDF membranes manufactured on a glass sheet or non-woven (~70°). However, considering the low porosity of the 3DP substrates (~21.7%), the PVDF coated 3DP (PVDF@3DP) membranes are found to have relatively low porosities at a range of 45%-62%. Furthermore, the high thickness of the PA substrates of 359.6±38.9 μm lead to relatively thick composite membranes, especially for the PVDF@3DP-10 membranes of ~500 μm. Therefore, the PVDF@3DP membranes had relatively low fluxes of around 10 kg/(m2·h) at a temperature difference of 40 °C with a feed temperature of 60 °C. The overall results indicate that the 3DP substrates significantly affect the MD performance of the composite membranes rather than the thin PVDF layer. Therefore, improving the porosity and decreasing the thickness of the printed substrates will be advantageous to prepare membranes with MD performance comparable to traditional membranes with quick fabrication and less solvent discharge. Secondly, a facile bottom-up method using water as coagulation bath was proposed to fabricate porous PVDF membranes. By covering a piece of non-woven substrate on the nascent film on a glass plate followed by immersion into a water bath, isotropic and skinless PVDF membranes were obtained. The SEM characterization confirms the formation of a rough top surface and sponge-like granular membranes composed of spherulites. The water contact angles substantially increase from 71.7° for conventional PVDF-N membrane to ca. 144° for bottom-up membranes. The DCMD flux of the bottom-up PVDF membrane is as high as 41.4 kg/(m2·h) with a polymer concentration of 15 wt.% when the feed and permeate temperatures were 70 °C and 20 °C, respectively. Furthermore, porous PVDF membranes with sponge-like structure were also developed in a co-casting process. Unlike the dual-layer membranes in which dual-layers attached tightly after co-casting, the attainment of independent PVDF membranes with uniformly rough surface structures necessitates the delamination of top-layer membranes from the underlying PVDF membranes. The coverage of top-layer membranes via co-casting is expected to reduce the solvent/nonsolvent exchange rate for the underlying PVDF membranes during a phase inversion process. In this context, a polyethersulfone (PES) membrane is co-cast onto a PVDF membrane followed by phase inversion in a water bath to fabricate PVDF membranes. The spontaneous delamination of PES from PVDF membranes occurs once the top-layer PES membrane solidifies. Due to the combined effect of the additional PES layer and the solvent retained at the PES/PVDF interface, delayed liquid-liquid (L-L) demixing of the PVDF solution take place, resulting in the formation of a porous surface with symmetric cross-section. Results show that the PVDF concentration significantly affects the membrane morphology. Increasing the PVDF content from 16 wt.% to 20 wt.% leads to a marked morphological change for membrane cross-section from cellular pores to PVDF globules, which indicates that the phase inversion mechanism varies from delayed L-L demixing to solid-liquid (S-L) demixing; this is mainly affected by the solution viscosity. Due to the roughness increment by the particulate surfaces, the hydrophobicity of PVDF-co membranes is distinctly enhanced. Furthermore, the membrane mean pore size is enlarged, and the PVDF layer thickness is reduced. Therefore, the PVDF-co membranes have much higher fluxes of 20.1-23.8 kg/(m2·h) in comparison to the single-layer PVDF membranes of 12.5- 6.5 kg/(m2·h) at feed and permeate temperatures of 60 °C and 20 °C, respectively, especially for PVDF-co membranes composed of PVDF particles which shows superior pore interconnectivity than the cellular pores. A long-term stability test was conducted with the PVDF-20-21 membrane for 50 h using a 3.5 wt.% NaCl solution as feed at a temperature difference of 40 °C. Fairly steady fluxes are observed over the testing course, as well as a continuous high salt rejection of above 99.9%.