The Impact of Thermal History on the Suitability of Polyamide 12 for Laser Sintering
Author:
Abstract:
In the 1980s, an innovative production technology called additive manufacturing (AM) was developed. Over the past decade, this technique has rapidly gained popularity, a trend which is underscored by a tenfold increase in global annual market revenues between 2012 and 2022. The inherent characteristics of AM, such as the high degree of design freedom, potential material savings, short time-to-market, and part specific tooling, are attracting the interest of both industry and academia. This interest extends beyond prototyping to the production of high performance, functional parts, with applications in the automotive, aerospace, engineering, medical, biological, and food sectors. Laser sintering (LS) is a standard polymer-based AM technique, categorized in the powder bed fusion group. The process involves the deposition of a layer of powder, followed by the sintering of the desired particles with a laser. Subsequent repetition of these steps allows to build an object in a layerwise fashion. An advantage of LS is the fact that no support material is required, as the unsintered powder in the build takes up this role. Disadvantages include the length of the printing process as well as the limited range of materials available. A polymer must meet specific requirements to ensure good part quality. As a result, polyamides, especially polyamide 12 (PA12), continue to dominate the material feedstock of LS, which is reflected by the amount of research dedicated to it. The good material performance of PA12 in terms of powder flow, laser absorption, thermal sintering window and rheological properties provide good coalescence and mechanical properties of the final part. However, some issues still need to be overcome to make laser sintering of PA12 a stable manufacturing process. A first challenge is the aging of polyamide 12 powder due to the LS process characteristics. Up to 85% of the material remains unsintered throughout the process, during which it is subjected to an elevated temperature for long periods of time. Accordingly, the post-condensation reaction alters the material properties of PA12, reducing the printability of the unsintered powder and, consequently, its recyclability for laser sintering. A second issue is the reproducibility of the final part properties, which is influenced by many parameters, both process and material related. The work presented in this dissertation focuses on the material side of the LS process. The aim of the study is to support the understanding of the origin of the limited powder recyclability and part reproducibility in order to optimize the laser sintering of PA12 to reduce the amount of waste and the number of failed printed parts, while still ensuring an excellent final quality. This research was conducted as part of the industry-focused GreenAM project, which aims to improve the sustainability of additive manufacturing technologies. The first part of this dissertation consists of a more general, fundamental investigation of how the thermal history given to PA12 can lead to physical or chemical changes in the material. The focus lies on comprehending the influence of these changes, referred to as memory effects, on crystallization kinetics. Understanding this could help to identify and predict changes in the crystallization behavior of PA12 as a function of the material's thermal history and the processing technique used. Three potential memory effects were investigated using differential scanning calorimetry (DSC) measurements. The first effect is self-nucleation by the action of crystalline residues, the second effect is chemical post-condensation in both the solid and the melt states, and the final effect is polymer chain disentangling and re-entangling. Self-nucleation and disentangling are confirmed to promote crystallization, while post-condensation and re-entangling hinder it. The significance of these effects is demonstrated by the 30 °C decrease in crystallization temperature obtained by establishing a specific thermal history that drives the interplay of these memory effects to an extreme. Particularly interesting for laser sintering is the impact of solid-state post-condensation at temperatures comparable to the standard bed temperature. The results show that on different timescales, this memory effect yields opposite outcomes. On short timescales (< 1 hour) the typical crystallization inhibiting effect of post-condensation dominates, while on long timescales (> 1 hour) crystal perfection and chain rearrangement happen, leading to the appearance of non-crystalline self-nucleating remnants in the melt, which only relax after more than one hour above the equilibrium melting temperature of PA12. This finding may be relevant in unravelling the differences in material properties between fresh and recycled PA12 powder from laser sintering. Subsequently, the second part of this thesis is more closely connected to the challenges associated with laser sintering, namely the limited reproducibility of part quality. The focus here is twofold. Over time, several theories have been proposed regarding the potential temperature profile and thus crystallization kinetics experienced by PA12 during laser sintering. Results ranged from (quasi-)isothermal crystallization during the cooling step to (non-)isothermal crystallization during the building step. However, these conclusions were all based on models or indirect DSC measurements. Therefore, realistic temperature profiles were first determined by means of in-situ thermocouple measurements during laser sintering and then imposed on PA12. Temperature profiles were established for a single set of process parameters, but for different locations within a printed part (e.g., bottom or top side) and for different bed temperatures. The crystallinity evolution and morphology of PA12 not prone to post-condensation, called endcapped PA12, was then followed by fast scanning calorimetry (FSC) to allow realistic heating and cooling rates, and microscopy. It is found that different locations in a printed part are subjected to a separate thermal history, thereby resulting in a variety of crystallization trajectories and morphologies. Although the final crystallinity is constant throughout a part, an inhomogeneous crystallization process, ranging from non-isothermal to isothermal crystallization or a combination of both, are observed as well as significant differences in spherulite size along the height of a printed part. In addition, small bed temperature variations do not significantly change the material behavior during laser sintering. On the contrary, further reduction of the bed temperature leads to a more homogeneous crystallization and morphology via non-isothermal crystallization. This adapted process, however, would introduce new issues with part density and coalescence. The final part of this dissertation features the bridge between the previous two parts. First, the knowledge of the crystallization behavior of PA12 during laser sintering is extended by a study of standard, non-endcapped PA12. The data were supplemented with combined WAXS-FSC-microscopy measurements for additional verification. In summary, the same conclusions regarding thermal behavior and morphology apply to both endcapped and non-endcapped PA12 subjected to the LS process. Additionally, PA12 was found to crystallize in the alpha'-phase regardless of the thermal protocol imparted during LS. Secondly, the influence of post-condensation and the use of aged powder on the crystallization of PA12 was investigated. As a result of solid-state annealing, non-crystalline remnants surviving above the equilibrium melting temperature lead to an altered crystallization pathway compared to fresh PA12 powder. It is hypothesized that the self-nucleation effect in aged powder increases the nucleation density, resulting in smaller spherulites. This could have an impact on the mechanical properties of aged PA12. It is also concluded that lowering the bed temperature to 120 °C could prevent aging of unsintered PA12 by post-condensation, although implementing this in the current LS process would present new challenges. In summary, this research provides a fundamental basis for understanding the inherent material behavior of PA12 under different thermal conditions and offers further insights into the potential for improving the sustainability of laser sintering.